University of Groningen
Atomic layer deposition of SiO2-GeO2 multilayers
Antoja Lleonart, Jordi; Zhou, Silang; de Hond, Kit; Huang, Sizhao; Koster, Gertjan; Rijnders,
A.J.H.M. (Guus); Noheda, Beatriz
Published in:
Applied Physics Letters
DOI:
10.1063/5.0009844
IMPORTANT NOTE: You are advised to consult the publisher's version (publisher's PDF) if you wish to cite from
it. Please check the document version below.
Document Version
Publisher's PDF, also known as Version of record
Publication date:
2020
Link to publication in University of Groningen/UMCG research database
Citation for published version (APA):
Antoja Lleonart, J., Zhou, S., de Hond, K., Huang, S., Koster, G., Rijnders, A. J. H. M. G., & Noheda, B.
(2020). Atomic layer deposition of SiO2-GeO2 multilayers. Applied Physics Letters, 117(4), [041601].
https://doi.org/10.1063/5.0009844
Copyright
Other than for strictly personal use, it is not permitted to download or to forward/distribute the text or part of it without the consent of the author(s) and/or copyright holder(s), unless the work is under an open content license (like Creative Commons).
Take-down policy
If you believe that this document breaches copyright please contact us providing details, and we will remove access to the work immediately and investigate your claim.
Downloaded from the University of Groningen/UMCG research database (Pure): http://www.rug.nl/research/portal. For technical reasons the number of authors shown on this cover page is limited to 10 maximum.
multilayers
Cite as: Appl. Phys. Lett. 117, 041601 (2020); https://doi.org/10.1063/5.0009844
Submitted: 03 April 2020 . Accepted: 09 July 2020 . Published Online: 28 July 2020
Jordi Antoja-Lleonart , Silang Zhou, Kit de Hond , Sizhao Huang, Gertjan Koster , Guus Rijnders, and Beatriz Noheda
Atomic layer deposition of SiO
2
–GeO
2
multilayers
Cite as: Appl. Phys. Lett. 117, 041601 (2020);doi: 10.1063/5.0009844
Submitted: 3 April 2020
.
Accepted: 9 July 2020.
Published Online: 28 July 2020JordiAntoja-Lleonart,1,a) SilangZhou,1Kitde Hond,2 SizhaoHuang,2GertjanKoster,2 GuusRijnders,2
and BeatrizNoheda1,b)
AFFILIATIONS
1Zernike Institute for Advanced Materials, University of Groningen, 9747AG Groningen, The Netherlands 2MESAþ Institute for Nanotechnology, University of Twente, PO Box 217, 7522 NH Enschede, The Netherlands
a)Electronic mail:j.antoja.lleonart@rug.nl
b)Author to whom correspondence should be addressed:b.noheda@rug.nl
ABSTRACT
Despite its potential for CMOS applications, atomic layer deposition (ALD) of GeO2thin films, by itself or in combination with SiO2, has
not been widely investigated yet. Here, we report the ALD growth of SiO2/GeO2multilayers on si1icon substrates using a so far unexplored
Ge precursor. The characterization of multilayers with various periodicities reveals layer-by-layer growth with electron density contrast and the absence of chemical intermixing, down to a periodicity of two atomic layers.
VC 2020 Author(s). All article content, except where otherwise noted, is licensed under a Creative Commons Attribution (CC BY) license (http://
creativecommons.org/licenses/by/4.0/).https://doi.org/10.1063/5.0009844
In the last four decades, atomic layer deposition (ALD) has seen widespread adoption as a thin film growth technique.1,2Its scalability, unprecedented conformality, and thickness control down to the atomic level make it a valuable asset to most nanofabrication efforts, playing a key role in commercial semiconductor manufacturing. Although chiefly known for the growth of relatively simple com-pounds, such as binary oxides, nitrides, or sulfides, amorphous for the most part, ALD is also used to grow metals,3and recently, more
com-plex, multicomponent materials,4,5 including perovskites,6–10 have been realized as well.
One of the materials with the longest history using the ALD tech-niques is SiO2,11a key element in the microelectronics industry with
applications as a passivation layer and gate oxide, among others. Less ubiquitous is the ALD growth of the related material GeO2; its growth
using ALD is relatively unexplored, and not many of its possible pre-cursors have been tested.12–14Research on GeO2films has been mainly
devoted to the study of the GeO2/Ge interface, with GeO2films being
proposed as a means to reduce the concentration of interface states between Ge and a high-K dielectric on top,15–17with the goal of
realiz-ing MOSFETs with a Ge-based channel. In these studies, thermal or plasma oxidation, as well as vapor growth,18,19was used. It is worth mentioning that these works use precursors containing alkoxy or halide ligands, which, in SiO2ALD, have been shown to have
less-than-ideal reactivity and corrosive byproducts.20,21
Thin films consisting of SiO2and GeO2multilayers have been
investigated in the past, from both solution and vapor deposition
methods,22–24with the focus being mostly on their optical properties. In this work, we show that using tetrakis(dimethylamino)germanium (IV) (TDMAGe) as a precursor, it is possible to deposit GeO2as well
as SiO2/GeO2 multilayers by thermal ALD. Proper intermixing
between SiO2and GeO2 in ALD multilayers is a key goal of this
growth experiment. Achieving intermixing via post-annealing is not an option, given that these two compounds are known to phase sepa-rate, rather than mix, upon heating.25,26
We use a Picosun R-200 Advanced hot-wall ALD System whose chamber opens to a glovebox containing a nitrogen atmosphere, with controlled oxygen and water concentrations. We grow oxide thin films using organometallic Si and Ge precursors. These are bis(diethylami-no)silane (BDEAS, commonly known as SAM-24) and TDMAGe, respectively, both of them purchased from Air Liquide. The precursors are housed in PicohotTM 300 and PicohotTM 200 canisters, which allow heating up to 260C and 200C, respectively. The organometal-lic precursors are delivered into the reaction chamber, through heated valve blocks, using nitrogen as carrier gas.
The oxidizer used in this work is ozone, which is produced from an INUSA Ozone Generator using Oxygen 6.0. Our valves allow a minimum opening time of 0.1 s. Accessible process temperatures range from 100C to 300C, and the typical process pressure is
17 hPa. A temperature of 38C for the BDEAS precursor bottle was established to give acceptable delivery rates. The TDMAGe bottle needed to be heated to 80C to achieve similar precursor delivery rates to the reaction chamber. The gas lines downstreaming from the bottles
Appl. Phys. Lett. 117, 041601 (2020); doi: 10.1063/5.0009844 117, 041601-1
VCAuthor(s) 2020
were heated to 10–20C above the temperature of their respective
bot-tle to avoid precursor condensation taking place before reaching the reaction chamber.
The SiO2growth from BDEAS was optimized in collaboration
with PicosunVR
. The reactor temperature was set to 300C. The
BDEAS pulse length was 0.1 s, followed by a 6.0 s N2purge. The ozone
pulse length was 8.0 s, also followed by a 6.0 s N2purge. In our system,
SiO2grown in this way shows a growth per cycle (GPC) of about
0.7 A˚ . The GeO2growth has been independently optimized in the
pre-sent work, as detailed below. The films are grown on 15 15 mm2 square pieces of Si(100) wafers purchased from Microchemicals GmbH.
Although the growth of GeO2 by ALD using TDMAGe as a
precursor was recently patented,14the details of the growth were not
reported. Even though the precursors used for GeO2and SiO2are
quite different, both of them use alkylamine ligands. This allowed us to optimize the GeO2growth, using as starting parameters those of the
SiO2growth.
In the case of the combined SiO2/GeO2multilayer growth, there
are practical constraints to the process. First, the well-known SiO2
pre-cursor BDEAS,27–32requires ozone or oxygen to function properly in thermal ALD. If water vapor is used instead, the Si–H bonds in the precursor do not react, which results in a decreased growth rate, possi-bly leading to too high impurity concentrations in the film. For this reason, it is highly desirable to simplify the process by using ozone as the oxidizer in GeO2growth as well, even though this may lead to
combustion-like reactions and less gentle oxidization. The ozone pulse length was fixed at 8 s, sufficient to ensure a complete half-reaction.
Second, the SiO2growth is optimal at or above 300C. When
growing subsequent layers of different materials by ALD, it is, in prin-ciple, possible to change the reaction temperature when switching from one oxide to the next. However, cooling and heating the reactor, even for relatively small temperature differences, are slow processes, making the growth time prohibitively long if the temperature needs to be changed repeatedly. For this reason, while the optimal growth temperature for pure GeO2 is determined, if GeO2 growth is still
acceptable at 300C, this temperature needs to be maintained in the
multilayer growth.
The minimum operating temperature of our system is, for this process, about 100C. This is necessary to avoid condensation of the precursors or their reaction products in the chamber. Its maximum operating temperature is 300C in its current configuration. Within this range, the growth rate of pure GeO2 increases with increasing
temperature, remaining approximately invariant above 150C
([Fig. 1(b)]. One explanation for this behavior is that below 150C,
the chemisorption reaction rate for TDMAGe is too low for proper ALD behavior, resulting in a decreased GPC. It could be argued that the stabilization of the GPC up to 300C is an indication that
precur-sor decomposition is still not significant at that temperature.
The GPC dependence on the pulse length was analyzed as well. The purge times were kept constant for this series. We can see that the GPC at 300C increases for longer TDMAGe pulses [Fig. 1(d)], while displaying approximately constant values for the short pulse lengths of 0.1 s and 0.2 s. This could indicate that this temperature is, in fact, suf-ficient to cause noticeable precursor decomposition, but that this has no noticeable effect in the growth, provided that the TDMAGe pulses are short enough. This was confirmed by growing a film at 200C
using TDMAGe pulses of 0.5 s. In that case, the GPC was 0.53 A˚ . This shows that the effect of precursor decomposition on the thickness can be minimized either by growing at sufficiently low temperatures, which is difficult in our case, as discussed before, or by keeping the pulse length short. Therefore, the shortest pulse length of 0.1 s was chosen. We further show, for large pulse numbers, the dependence of the film thickness on the number of pulses [Fig. 1(c)].
The dielectric properties of GeO2films grown with the optimized
parameters were also investigated.Figure 2shows the result of several capacitance measurements on one of these films. At low frequencies, we observe a Debye relaxation with a characteristic time of 6 ms, which was determined from fitting the real component of the permittivity (e0r). This likely corresponds to space charge relaxation. The relative
dielectric constant at 1 kHz is e0r¼ 22.
The dielectric constant value that we have determined at 1 kHz is significantly larger than those available in the literature, such as the
FIG. 1. (a) Sketch of the pulse trains of the two precursors. (b) GeO2film thickness
after 100 cycles at various reactor temperatures. (c) GeO2film thickness for
differ-ent cycle numbers, at 300C. A linear regression for this regime yields a GPC of 0.51 A˚. (d) GeO2film thickness for 100 cycles and at 300C for different TDMAGe
pulse lengths. Error bars are estimated based on sample dispersion.
FIG. 2. Relative dielectric constant (real and imaginary) for a 12 nm GeO2film as
calculated from C–V measurements between 1 Hz and 5 KHz. The tan(d) value is below 1 for all points above 300 Hz. Dispersion between successive measurements is most visible at low frequencies. The red lines are a Debye fit with s¼ 6 ms.
theoretical value of e0
r 2.8 extrapolated by Walker et al.,33the
experi-mentally determined static e0
rbetween 5 and 7 for GeO2grown by Ge
oxidization,34,35 or the near-static value of e0
r 8.5 for
vacuum-evaporated films.36 Some GeO2 crystalline phases have also been
explored,37–39with their e0
r being significantly different for different
phases. We have also determined the dielectric constant by spectro-scopic ellipsometry in the range of 300–1700 nm (see the supplemen-tary material). These results reveal a high-frequency e0
r 2, slightly
smaller than literature sources.40–43This suggests at least one more relaxation process between 5 kHz and the near-infrared (NIR) range. This relaxation can be of the dipole polarization of small amounts of absorbed water, as GeO2is known to be hygroscopic.44
We then proceeded to grow multilayer heterostructures with alternating SiO2and GeO2sublayers. This multilayer approach has
been often utilized to synthesize complex materials by ALD.4This lay-ered growth is often characterized in the literature by the ratio between the numbers of pulses of the metal precursors of the two components. Here, we have synthesized multilayers with different SiO2/GeO2
perio-dicities using a constant 1:1 pulse ratio and the same total number of pulses (the same total thickness), but varying the number of pulses in each train. In this way, it is possible to control the degree of intermix-ing durintermix-ing the growth step, without resortintermix-ing to post-annealintermix-ing.
For the experiments here, we set the total number of cycles to 300, of which half will be GeO2and the other half SiO2. Note that,
assuming that the behavior displayed inFig. 1(c)can be extrapolated to lower cycle numbers, the expected thickness for the GeO2and SiO2
layers would be 8 nm and 11 nm, respectively, taking into account our previously mentioned GPC values at the optimized process parame-ters. Thus, assuming an ALD linear regime, we expect a total thickness of 19 nm approximately, without accounting for the native oxide pre-sent on the wafer. This is in good agreement with the values obtained from the fitting of the XRR patterns, which give total thicknesses rang-ing between 19.2 nm and 20.1 nm (see Table S1 in thesupplementary material).
The first experiment, with 150 cycles of TDMAGe/O3followed
by 150 cycles of BDEAS/O3, is denoted as “one repetition” (seeFig. 3).
One repetition, thus, contains a GeO2sublayer and a SiO2sublayer. In
the following experiments, the number of cycles in each sublayer is subsequently halved, while the number of repetitions is doubled in order to keep the total number of pulses constant. The XRR patterns of these films, their fits and an illustration of the models used in the fits, are plotted inFig. 4(the actual parameters of the model can be found in Table S1 of thesupplementary material). By differentiating the experimental data (which has been obtained with a step size of 0.01 in 2h) at low angles and smoothing it with a Savitzky–Golay filter, we determined the critical angle for all the films to be 0.235 60.005, independent of the number of repetitions (or the periodicity of the multilayer), close to the bulk value for SiO2(0.234for a density
of 2.65 g/cm3).
The XRR patterns show clear thickness oscillations in all cases, indicating the good homogeneity of the films and the quality of the top and bottom interfaces. In addition, the patterns corresponding to the films containing from 2 up to 15 repetitions all display superlattice reflections, attesting for the presence of chemical contrast between the SiO2and GeO2sublayers.
The XRR pattern of the film with 15 repetitions shows its super-lattice signature peak at about 7.1, corresponding to a period of 12 A˚ ,
which is approximately the size of two unit cells in SiO2and GeO2
crystalline polymorphs. In the case of the 15 repetitions sample, despite the clear superlattice peak, the model is not able to provide a reliable value for the thickness of the individual SiO2or GeO2
sub-layers. This can be understood looking at the roughness values (see Table S1 in thesupplementary material), which are of the order of the estimated sublayer thickness (6 A˚ ). For the 30 repetition film, only 5 pulses were provided, alternately, for each SiO2and GeO2sublayer,
until the total of 300 pulses is complete. Therefore, the superlattice periodicity is expected to be half of the value of the periodicity displayed by the 15 repetition films, 6 A˚ . This value is similar to the
FIG. 3. (a) Schematic representation of the synthesis method for the mixed oxide films. In our study, the pulse trains for the two precursors contain the same number of pulses: nTDMAGe¼ nBDEAS¼ n, and it varies from film to film. (b) Table detailing
the number of precursor pulses in each train (n) per sublayer and the total number of cycles (N) in the different films. For the 1:1 pulse ratio used in this work, the total number of cycles (2n N) was kept to approximately 300 for the whole series. This means that for the 1 repetition case, 150 cycles of TDMAGe/O3were done,
and after that came 150 cycles of BDEAS/O3, for a total of 300 cycles in two layers.
(c) Sketch of the expected layered structure after growth.
FIG. 4. (a) XRR scans and fits (red dashed lines) of the six films, from which the thicknesses were extracted. (b) Side view of the grown films, showing the actual layer thicknesses as determined by XRR. The red and blue stripes indicate layers made of different oxides, whereas the purple stripe is used for a layer of mixed oxide. Superlattice fits add the constraint that all SiO2layers and all GeO2layers in
a single heterostructure have the same thickness, but this constraint is relaxed for the top SiO2and the bottom GeO2layer in each case, respectively. The native
SiO2layers, although both measured by ellipsometry prior to the ALD process and
accounted for in the models, are not depicted here. Note that the models do include interface roughnesses. The right axis shows the thickness in multiples of 0.55 nm, which is approximately the average between the SiO2and GeO2a-quartz of the
c-parameter, as it is used as a characteristic length scale of the material (though it is amorphous in this case).
Applied Physics Letters
ARTICLE scitation.org/journal/aplAppl. Phys. Lett. 117, 041601 (2020); doi: 10.1063/5.0009844 117, 041601-3
roughness values obtained with the reflectivity fit, and thus, no chemi-cal contrast is expected. Indeed, in this case, the superlattice model also gives unreliable results, but, unlike in the case of the 15 repetition film, the 30 repetition XRR pattern can be modeled by a uniform layer (see Table S1 in the supplementary material), consistent with the absence of superlattice peaks up to an angle of 14.
The model roughness values are in agreement with those deter-mined by AFM (RMS roughness).Figure 5 shows a representative AFM image of a sample surface. AFM micrographs of the six multi-layer types are available in thesupplementary material, as are the AFM roughnesses, in Table S1. In addition, x-ray Photoelectron Spectroscopy (XPS) on these films has shown small amounts of carbon contamination in the films (see thesupplementary material), most likely arising from the ALD growth process.
From this series of experiments, it becomes clear that electron density, or composition, contrast between the SiO2and the GeO2
sub-layers is present down to the atomic level (close to a unit cell of their stable polymorphs). On the one hand, these results attest the excellent capabilities of ALD in general, allowing the growth of heterostructures with atomic-scale thickness control. On the other hand, it nicely illus-trates a potential pitfall of the layered approach to compositional tun-ing in ALD, in that extremely short supercycles are needed in order to achieve a uniform composition rather than a superlattice.
As a final note, it must be pointed out that, as directly visible in
Fig. 4, the SiO2:GeO2thickness ratio, and therefore the atomic ratio,
changes from one film to the next, even though the pulse ratio for all of them is maintained at 1:1. This dependence of the composition on the precise pulsing sequence, and not only on the pulse ratio, has been previously observed.45
To conclude, we have optimized the ALD growth of GeO2thin
films from TDMAGe and O3precursors. In order to achieve SiO2/
GeO2 films by sequential layered growth, a compromise has been
found between the optimal growth parameters and those parameters that will allow us to synthesize a mixed oxide film in a reasonable amount of time. Armed with this knowledge, we have set out on the synthesis of a series of increasingly intermixed SiO2/GeO2thin films,
showing that ALD indeed is able to achieve atomic level accuracy for these compounds as well.
See thesupplementary materialfor further details on the experi-mental methods, high-frequency ellipsometry-determined dielectric constants, AFM images of the films, and details and fitting parameters giving rise to the XRR simulation curves inFig. 4.
The authors are grateful to PicosunVR
for their optimization report related to the growth of SiO2, to Adrian Carretero-Genevrier
and Vaclav Ocelık for useful discussions, and to Ir. Jacob Baas and the Zernike NanoLab Groningen for the technical support. The authors also acknowledge financial support from NWO’s TOP-PUNT Grant No. 718.016002.
DATA AVAILABILITY
The data that support the findings of this study are available from the corresponding author upon reasonable request.
REFERENCES
1R. L. Puurunen,J. Appl. Phys.97, 121301 (2005). 2
R. W. Johnson, A. Hultqvist, and S. F. Bent,Mater. Today17, 236 (2014).
3J. H€am€al€ainen, M. Ritala, and M. Leskel€a,Chem. Mater.26, 786 (2014). 4
A. J. Mackus, J. R. Schneider, C. Macisaac, J. G. Baker, and S. F. Bent,Chem. Mater.31, 1142 (2019).
5
M. Coll and M. Napari,APL Mater.7, 110901 (2019).
6
M. Tyunina, M. Plekh, J. Levoska, M. Vehkam€aki, M. Hatanp€a€a, M. Ritala, and M. Leskel€a,Integr. Ferroelectr.102, 29 (2008).
7
N. M. Sbrockey, M. Luong, E. M. Gallo, J. D. Sloppy, G. Chen, C. R. Winkler, S. H. Johnson, M. L. Taheri, G. S. Tompa, and J. E. Spanier,J. Electron. Mater. 41, 819 (2012).
8A. R. Akbashev, G. Chen, and J. E. Spanier,Nano Lett.14, 44 (2014). 9
M. D. McDaniel, T. Q. Ngo, S. Hu, A. Posadas, A. A. Demkov, and J. G. Ekerdt,Appl. Phys. Rev.2, 041301 (2015).
10E. L. Lin, A. B. Posadas, L. Zheng, J. E. Ortmann, S. Abel, J. Fompeyrine, K. Lai,
A. A. Demkov, and J. G. Ekerdt,J. Appl. Phys.126, 064101 (2019).
11Note1. Occasionally “pulsed metal organic chemical vapor deposition” is used
instead of ALD, though in practice both methods are very similar.
12
P. R. Chalker, P. A. Marshall, P. J. King, K. Dawson, S. Romani, P. A. Williams, J. Ridealgh, and M. J. Rosseinsky,J. Mater. Chem.22, 12824 (2012).
13V. Adinolfi, L. Cheng, M. Laudato, R. C. Clarke, V. K. Narasimhan, S. Balatti, S.
Hoang, and K. A. Littau,ACS Nano13, 10440 (2019).
14
R. H. Matero, “Atomic layer deposition of GeO2(US Patent)” 2014/0065841
A1 (2014).
15
T. Yoshida, K. Kato, S. Shibayama, M. Sakashita, N. Taoka, W. Takeuchi, O. Nakatsuka, and S. Zaima, Jpn. J. Appl. Phys., Part 1 53, 08LD03 (2014).
16S. Shibayama, T. Yoshida, K. Kato, M. Sakashita, W. Takeuchi, N. Taoka, O.
Nakatsuka, and S. Zaima,Appl. Phys. Lett.106, 062107 (2015).
17
M. Kanematsu, S. Shibayama, M. Sakashita, W. Takeuchi, O. Nakatsuka, and S. Zaima,Jpn. J. Appl. Phys., Part 155, 08PC05 (2016).
18H. Matsubara, T. Sasada, M. Takenaka, and S. Takagi,Appl. Phys. Lett.93,
032104 (2008).
19J. Robertson and R. M. Wallace,Mater. Sci. Eng., R88, 1 (2015). 20
J. Bachmann, R. Zierold, Y. T. Chong, R. Hauert, C. Sturm, R. Schmidt-Grund, B. Rheinl€ander, M. Grundmann, U. G€osele, and K. Nielsch,Angew. Chem., Int. Ed.47, 6177 (2008).
21M. Putkonen, M. Bosund, O. M. E. Ylivaara, R. L. Puurunen, L. Kilpi, H.
Ronkainen, S. Sintonen, S. Ali, H. Lipsanen, X. Liu, E. Haimi, S. P. Hannula, T. Sajavaara, I. Buchanan, E. Karwacki, and M. V€ah€a-Nissi,Thin Solid Films558, 93 (2014).
22Q. Y. Zhang, K. Pita, C. K. F. Ho, N. Q. Ngo, L. P. Zuo, and S. Takahashi,
Chem. Phys. Lett.368, 183 (2003).
23
C. K. F. Ho, H. S. Djie, K. Pita, N. Q. Ngo, and C. H. Kam,Electromech. Solid-State Lett.7, F96 (2004).
24C. K. F. Ho, K. Pita, N. Q. Ngo, and C. H. Kam,Opt. Express13, 1049 (2005).
25H. Hosono and J. Nishii,Opt. Lett.24, 1352 (1999). 26
K. Sasan, A. Lange, T. D. Yee, N. Dudukovic, D. T. Nguyen, M. A. Johnson, O. D. Herrera, J. H. Yoo, A. M. Sawvel, M. E. Ellis, C. M. Mah, R. Ryerson, L. L. Wong, T. Suratwala, J. F. Destino, and R. Dylla-Spears,ACS Appl. Mater. Interfaces12, 6736 (2020).
27
S.-J. Won, S. Suh, M. S. Huh, and H. J. Kim,IEEE Electron Device Lett.31, 857 (2010).
28
M. L. O’Neill, H. R. Bowen, A. Derecskei-Kovacs, K. S. Cuthill, B. Han, and M. Xiao,Electrochem. Soc. Interface20, 33 (2011).
29
S. B. Baek, D. H. Kim, and Y. C. Kim,Appl. Surf. Sci.258, 6341 (2012).
30A. Mallikarjunan, H. Chandra, M. Xiao, X. Lei, R. M. Pearlstein, H. R. Bowen,
M. L. O’Neill, A. Derecskei-Kovacs, and B. Han,J. Vac. Sci. Technol., A33, 01A137 (2015).
31
G. Fang, L. Xu, J. Ma, and A. Li,Chem. Mater.28, 1247 (2016).
32M. C. Schwille, T. Sch€ossler, F. Sch€on, M. Oettel, and J. W. Bartha,J. Vac. Sci.
Technol., A35, 01B119 (2017).
33B. Walker, C. C. Dharmawardhana, N. Dari, P. Rulis, and W. Y. Ching,J.
Non-Cryst. Solids428, 176 (2015).
34F. Bellenger, M. Houssa, A. Delabie, T. Conard, M. Caymax, M. Meuris, K. D.
Meyer, and M. Heyns,ECS Trans.11, 451 (2019).
35S. Takagi, T. Maeda, N. Taoka, M. Nishizawa, Y. Morita, K. Ikeda, Y.
Yamashita, M. Nishikawa, H. Kumagai, R. Nakane, S. Sugahara, and N. Sugiyama,Microelectron. Eng.84, 2314 (2007).
36
I. Banu Lucy,J. Mater. Sci.42, 5875 (2007).
37D. M. Roessler and W. A. Albers,J. Phys. Chem. Solids33, 293 (1972). 38
C. Sevik and C. Bulutay,J. Mater. Sci.42, 6555 (2007).
39M. Tamura, J. Nakamura, and A. Natori,Key Eng. Mater.470, 60 (2011). 40
J. W. Fleming,Appl. Opt.23, 4486 (1984).
41T. N. Nunley, N. S. Fernando, N. Samarasingha, J. M. Moya, C. M. Nelson, A.
A. Medina, and S. Zollner,J. Vac. Sci. Technol., B34, 061205 (2016).
42G. G. Devyatykh, E. M. Dianov, N. S. Karpychev, S. M. Mazavin, V. M.
Mashinski K%, V. B. Neustruev, A. V. Nikola K%chik, A. M. Prokhorov, A. I. Ritus, N. I. Sokolov, and A. S. Yushin,Sov. J. Quantum Electron.10, 900 (1980).
43L. Pajasova,Czech. J. Phys.19, 1265 (1969). 44
S. R. Da Silva, G. K. Rolim, G. V. Soares, I. J. Baumvol, C. Krug, L. Miotti, F. L. Freire, M. E. Da Costa, and C. Radtke,Appl. Phys. Lett.100, 191907 (2012).
45V. Longo, N. Leick, F. Roozeboom, and W. M. M. Kessels,ECS J. Solid State
Sci. Technol.2, N15 (2013).
Applied Physics Letters
ARTICLE scitation.org/journal/aplAppl. Phys. Lett. 117, 041601 (2020); doi: 10.1063/5.0009844 117, 041601-5